Glazing is the step people ask us about most, and the one we rush least. A glaze is a thin layer of glass fused to the clay at 2,264 °F. Get it right and the surface stays food-safe and dishwasher-proof for decades.
Two firings, not one
Every piece is bisque fired first, to 1,832 °F. That leaves the clay hard enough to handle but porous enough to drink up glaze evenly. Then comes the part that takes practice:
Wax the foot so the glaze stops 5 mm above the base.
Dip for a slow count of three. Thicker coats pool in the curve of a bowl and turn glossy.
Wipe, dry overnight, then load the glaze kiln shelf by shelf.
The kiln always has the last word. We just try to give it a good argument.
Ingrid Moe, studio lead
Our Fjord glaze is reactive, so no two mugs match exactly. That is why we stamp the batch code, such as FJ-26-09, on every foot.
Why every mug looks slightly different
The same glaze bucket can give three different results depending on where a piece sits in the kiln. Hotter shelves near the burners melt the glaze further, so the speckle spreads and the rim darkens.
Glaze recipes, by dry weight
Glaze | Finish | Base | Colourant |
|---|---|---|---|
Fjord | Satin | Feldspar, silica, whiting | Iron oxide 4% |
Oat | Matte | Dolomite, kaolin | Rutile 3% |
Slate | Gloss | Frit, silica | Cobalt 0.5% |
Our glaze firing schedule
Climb slowly to 1,112 °F so trapped water can escape.
Hold at 2,264 °F for 15 minutes to heal pinholes.
Segment Rate (°F/h) Target (°F) Hold (min)
1 180 1,112 0
2 270 2,012 0
3 110 2,264 15